As per ASME IX-2007,

If I weld two PQR's

PQR A is welded with SMAW to join 20mm thick plates with 20mm of thickness deposits.
PQR B is welded with GTAW and SMAW to join 20mm thick plates with 5mm of GTAW deposits and 15mm of SMAW deposits.

Question 1 :Do PQR's A and B qualify the SMAW WPS for the basic metal thickness range of 5 mm to 200 mm when impact testing is not required?

Question 2 :Do PQR B qualify the GTAW WPS for the basic metal thickness range of 1.5 mm to 10 mm when impact testing is not required?

Question 3 :Do PQR B qualify the combination(GTAW+SMAW) WPS for the basic metal thickness range of 5mm to 40mm when impact testing is not required?

If the above was right,i can qualify 3 WPS for the 2 PQR A & B.please advice.

_________________
Kareem


Top
 Profile  
 
PostPosted: Sun Jul 05, 2009 2:32 pm 
Offline
----------------
----------------

Joined: Tue Jan 29, 2008 5:00 pm
Posts: 103
Do PQR's A and B qualify the SMAW WPS for the basic metal thickness range of 5 mm to 200 mm when impact testing is not required?

No; qualification range will be 5- 40mm for base metal

Do PQR B qualify the GTAW WPS for the basic metal thickness range of 1.5 mm to 10 mm when impact testing is not required?

No; qualification range will be 5- 40mm for base metal and 10mm max for GTAW weld metal

Do PQR B qualify the combination(GTAW+SMAW) WPS for the basic metal thickness range of 5mm to 40mm when impact testing is not required?

Yes; qualification range will be max 10mm for GTAW and 30mm for SMAW

_________________
Raghuram


Top
 Profile  
 
Display posts from previous:  Sort by  
Post new topic Reply to topic  [ 2 posts ] 

All times are UTC + 2 hours


Who is online

Users browsing this forum: No registered users and 0 guests


You cannot post new topics in this forum
You cannot reply to topics in this forum
You cannot edit your posts in this forum
You cannot delete your posts in this forum
You cannot post attachments in this forum

Search for:
Jump to:  
Powered by phpBB® Forum Software © phpBB Group

phpBB SEO